November 16, 2026

M45 Concrete Mix Design as per IS 10262:2019

This article presents an illustrative initial trial mix design for M45 concrete using the general mix-proportioning procedure of IS 10262:2019.

The example is prepared for very-severe-exposure reinforced cement concrete, using OPC 53 cement, 20 mm crushed angular aggregate, 12.5 mm coarse aggregate, Zone II manufactured sand, a 100 mm target slump and a compatible superplasticizer.

M45 is a higher-grade concrete. It must not be produced by simply increasing the cement content of an M30 or M35 mix. The final mix must be verified using actual materials, laboratory trials and project requirements.

Page Contents

Important Engineering Note

This is an educational worked example and not a universal M45 concrete recipe.

The final mix must be confirmed using:

  • Actual cement properties
  • Aggregate grading and specific gravity
  • Aggregate moisture and absorption
  • Admixture compatibility
  • Required workability and slump retention
  • Trial-mix results
  • Cube compressive strength
  • Durability requirements
  • Project specifications
  • Approval by the responsible engineer

Do not use the calculated quantities directly for production without proper verification.

1. Mix Design Stipulations

PropertyAdopted value
Grade of concreteM45
Characteristic compressive strength at 28 days45 N/mm²
Exposure conditionVery severe exposure for RCC
Minimum RCC grade for selected exposureM35
CementOPC 53 grade
Mineral admixtureNone
Maximum nominal size of aggregate20 mm
Target slump100 mm
Concrete placementNormal, non-pumped placement
Degree of supervisionGood
Coarse aggregateCrushed angular aggregate
Fine aggregateManufactured sand, assumed Zone II
Chemical admixtureSuperplasticizer
Trial admixture dosage1.00% by mass of cement
Maximum free water–cement ratio0.45
Minimum cement content340 kg/m³
Adopted cement content410 kg/m³
Maximum cement-content check450 kg/m³
Aggregate conditionSaturated surface-dry
Assumed entrapped air1%

The selected exposure condition is used only for this worked example. The actual exposure classification must be established from the project environment and specifications.

2. Why the Exposure Condition Is Important

Concrete durability requirements depend on the exposure condition.

For the selected very-severe-exposure RCC condition, this example adopts:

  • Maximum free water–cement ratio = 0.45
  • Minimum cement content = 340 kg/m³
  • Minimum RCC grade = M35

Although M45 is higher than the minimum grade required for the selected exposure, the durability limits still apply.

For extreme exposure, the applicable requirements are more stringent. The mix must be redesigned if the exposure condition changes.

Plain concrete, reinforced concrete and prestressed concrete may have different requirements. Always check the latest applicable standards and project specifications.

3. Material Properties

3.1 Cement and Chemical Admixture

MaterialPropertyAdopted value
CementTypeOPC 53 grade
CementSpecific gravity3.15
SuperplasticizerTypeHigh-range water-reducing admixture
SuperplasticizerSpecific gravity1.09
Superplasticizer dosagePercentage by mass of cement1.00%

The superplasticizer dosage is only an initial trial assumption.

The manufacturer’s technical datasheet, recommended dosage range, compatibility, setting behaviour, slump retention and strength performance must be checked before use.

3.2 Aggregate Specific Gravity

AggregateSpecific gravity
20 mm coarse aggregate2.70
12.5 mm coarse aggregate2.70
Zone II manufactured sand2.65
Water1.00

The actual laboratory test values must be used for the final mix design.

3.3 Aggregate Moisture Condition

The main calculation is based on saturated surface-dry aggregate conditions.

Actual batching requires correction for:

  • Free surface moisture
  • Aggregate absorption
  • Stockpile condition
  • Rainfall or drying
  • Aggregate temperature
  • Batch-plant weighing accuracy

The quantities calculated in this article must not be used directly for production batching without moisture correction.

4. Target Mean Strength

The characteristic compressive strength of M45 concrete is:

fck = 45 N/mm²

When sufficient production test data are not available, the assumed standard deviation for this worked example is:

S = 5.0 N/mm²

The target mean strength is determined using:

f′ck = fck + 1.65S

and

f′ck = fck + X

For this M45 example, the grade-dependent margin is taken as:

X = 6.5 N/mm²

4.1 Calculation Using Standard Deviation

f′ck = fck + 1.65S

f′ck = 45 + (1.65 × 5.0)

f′ck = 45 + 8.25

f′ck = 53.25 N/mm²

4.2 Calculation Using Grade-Dependent Margin

f′ck = fck + X

f′ck = 45 + 6.5

f′ck = 51.50 N/mm²

The higher value is adopted.

Target mean strength = 53.25 N/mm²

The actual standard deviation should be calculated from project test results whenever sufficient production data become available.

5. Selection of Water–Cement Ratio

For the selected very-severe-exposure RCC condition:

Maximum permitted free water–cement ratio = 0.45

Because M45 requires a higher strength than M30, a lower initial water–cement ratio is selected for this worked example.

Adopted calculation-basis water–cement ratio = 0.36

The selected value is below the durability limit of 0.45.

The final water–cement ratio must satisfy:

  • Target mean strength
  • Durability requirements
  • Required workability
  • Aggregate grading
  • Cement characteristics
  • Admixture compatibility
  • Trial-mix strength results

The value of 0.36 is an initial trial value and is not a universal water–cement ratio for every M45 concrete mix.

6. Water Content Calculation

For 20 mm angular aggregate and a reference slump of 25–50 mm, the approximate water content is taken as:

Water content = 186 litres/m³

The required target slump is:

Target slump = 100 mm

Taking 50 mm as the reference slump, the increase is approximately 50 mm.

Using an approximate 3% increase for every 25 mm increase in slump:

Water increase = 3% × 2

Water increase = 6%

6.1 Water Before Admixture Reduction

Water = 186 × 1.06

Water = 197.16 litres/m³

Therefore:

Water before admixture reduction ≈ 197 litres/m³

6.2 Water Reduction Using Superplasticizer

For this illustrative calculation, approximately 25% water reduction is assumed through the use of a compatible superplasticizer.

Reduced water:

= 197.16 × 0.75

= 147.87 litres/m³

For consistency with the selected cement content and water–cement ratio:

External design water:

= 410 × 0.36

= 147.6 litres/m³

Therefore, adopt:

External design water = 147.6 litres/m³

For practical batching, this may be rounded to:

Approximately 148 litres/m³

The 25% water-reduction assumption is not a fixed code value. The actual reduction depends on:

  • Cement chemistry
  • Aggregate grading
  • Admixture type
  • Admixture dosage
  • Mixing time
  • Concrete temperature
  • Slump-retention requirement
  • Compatibility between cement and admixture

6.3 Water-Balance Note for Liquid Admixture

For this illustrative calculation, 147.6 litres/m³ is treated as the externally added design water.

The liquid superplasticizer is included separately by its mass and absolute volume.

The water contained in the liquid admixture is not included in the 147.6 litres/m³ figure because the product water content has not been specified.

For the final approved mix, obtain the admixture water content from the manufacturer’s datasheet and include it consistently in the effective water–cement ratio and absolute-volume calculation.

Do not count the same water twice.

7. Cement Content Calculation

The durability-based minimum cement content for the selected very-severe-exposure RCC condition is:

Minimum cement content = 340 kg/m³

The cement required for the selected water–cement ratio is:

Cement = Water ÷ Adopted water–cement ratio

Cement = 147.6 ÷ 0.36

Cement = 410 kg/m³

CheckCement quantity
Durability minimum340 kg/m³
Cement required at w/c = 0.36410 kg/m³
Adopted cement content410 kg/m³
Maximum cement-content check450 kg/m³

The adopted value is:

Cement content = 410 kg/m³

This value is above the durability minimum and below the assumed maximum cement-content check.

The adopted cement content is an initial trial value and must be confirmed through target-strength, workability, durability and trial-mix results.

7.1 Calculation-Basis Water–Cement Ratio

Calculation-basis water–cement ratio:

= External design water ÷ Cement

= 147.6 ÷ 410

= 0.36

The actual effective water–cement ratio must be checked after considering water contained in the liquid admixture and moisture contributed by aggregates.

8. Chemical Admixture Content

The superplasticizer dosage is assumed as 1.00% by mass of cement.

Admixture quantity:

= 410 × 1.00 ÷ 100

= 4.10 kg/m³

Therefore:

Superplasticizer = 4.10 kg/m³

8.1 Volume of Liquid Admixture

Volume of admixture:

= Mass ÷ (Specific gravity × 1000)

= 4.10 ÷ (1.09 × 1000)

= 0.00376 m³

Therefore:

Volume of superplasticizer ≈ 0.00376 m³

The final dosage must be checked against:

  • Manufacturer’s recommended dosage
  • Compatibility with OPC 53 cement
  • Slump and slump-retention requirements
  • Setting time
  • Bleeding and segregation
  • Trial-mix strength
  • Concrete temperature

The water contained in the liquid admixture must be checked separately against the final effective water–cement ratio.

9. Coarse and Fine Aggregate Proportioning

For 20 mm nominal maximum-size aggregate and Zone II fine aggregate, the reference coarse-aggregate fraction at a water–cement ratio of 0.50 is approximately:

Reference coarse-aggregate fraction = 0.62

The selected calculation-basis water–cement ratio is:

0.36

Difference:

0.50 − 0.36 = 0.14

Using an approximate adjustment of 0.01 for every 0.05 change in water–cement ratio:

Adjustment:

= (0.14 ÷ 0.05) × 0.01

= 0.028

Corrected coarse-aggregate fraction:

= 0.62 + 0.028

= 0.648

Therefore:

Coarse-aggregate fraction ≈ 0.648

Fine-aggregate fraction:

= 1.00 − 0.648

= 0.352

Therefore:

Fine-aggregate fraction ≈ 0.352

These are initial proportioning values. The final aggregate blend must be confirmed using:

  • Sieve analysis
  • Combined grading
  • Workability
  • Void-content assessment
  • Bleeding and segregation observations
  • Trial-mix results

10. Absolute Volume Calculation

The absolute-volume method is used for one cubic metre of concrete.

10.1 Volume of Cement

Volume of cement:

= Mass ÷ (Specific gravity × 1000)

= 410 ÷ (3.15 × 1000)

= 0.1302 m³

10.2 Volume of External Design Water

Volume of water:

= 147.6 ÷ (1.00 × 1000)

= 0.1476 m³

10.3 Volume of Superplasticizer

Volume of admixture:

= 0.00376 m³

10.4 Volume of Entrapped Air

For normal non-air-entrained concrete with 20 mm aggregate:

Entrapped air = 1%

Volume of air:

= 1 ÷ 100

= 0.010 m³

10.5 Volume Available for Aggregates

Volume of aggregates:

= 1 − (Volume of cement + Volume of water + Volume of admixture + Volume of air)

Volume of aggregates:

= 1 − (0.1302 + 0.1476 + 0.00376 + 0.010)

Volume of aggregates:

= 1 − 0.29156

Volume of aggregates ≈ 0.7085 m³

10.6 Coarse Aggregate Quantity

Volume of coarse aggregate:

= 0.7085 × 0.648

= 0.4591 m³

Mass of coarse aggregate:

= 0.4591 × 2.70 × 1000

= 1239.6 kg/m³

Therefore:

Coarse aggregate ≈ 1240 kg/m³

10.7 Fine Aggregate Quantity

Volume of fine aggregate:

= 0.7085 − 0.4591

= 0.2494 m³

Mass of fine aggregate:

= 0.2494 × 2.65 × 1000

= 660.9 kg/m³

Therefore:

Fine aggregate ≈ 661 kg/m³

11. Final Initial Trial Mix per Cubic Metre

MaterialQuantity per m³
OPC 53 cement410 kg
Fine aggregateApproximately 661 kg
Coarse aggregateApproximately 1240 kg
External design water147.6 litres
Practical rounded water valueApproximately 148 litres
Superplasticizer4.10 kg
Calculation-basis water–cement ratio0.36
Target slump100 mm
Entrapped airApproximately 1%

These quantities are based on assumed material properties and saturated surface-dry aggregates.

They represent an initial trial mix only. The final production mix must be adjusted after testing the actual materials.

12. Approximate Coarse Aggregate Split

For an initial combined coarse-aggregate blend, the following split may be used for trial purposes:

Aggregate sizeApproximate percentageQuantity
20 mm aggregate60%Approximately 744 kg
12.5 mm aggregate40%Approximately 496 kg
Total coarse aggregate100%Approximately 1240 kg

The 60:40 split is only an initial trial proportion.

The final blend must be selected using actual sieve analysis, combined grading, void content, workability and trial-mix results.

13. Approximate Mass-Based Trial Proportion

Taking cement as one part:

Cement : Fine aggregate : Coarse aggregate

410 : 661 : 1240

Dividing by 410:

1 : 1.61 : 3.02

This is an approximate calculated mass-based trial proportion.

It is not a fixed nominal volumetric ratio such as 1:2:4. It must not be treated as a universal M45 concrete mix.

14. Quantities for a 50-Litre Trial Batch

A 50-litre trial batch is equal to:

50 litres = 0.05 m³

MaterialQuantity for 50 litres
OPC 53 cement20.50 kg
Fine aggregate33.05 kg
Coarse aggregate62.00 kg
External design water7.38 litres
Practical rounded water valueApproximately 7.40 litres
Superplasticizer0.205 kg or 205 g

The plant water must be adjusted for aggregate moisture.

The liquid admixture must be weighed or measured accurately and added according to the approved trial procedure.

Use calibrated weighing equipment for trial batching. Do not estimate these quantities using uncalibrated volume containers.

15. Moisture and Absorption Correction

The calculated quantities are based on saturated surface-dry aggregate conditions.

For this simplified illustration, assume:

  • Fine aggregate free surface moisture = 3%
  • Coarse aggregate free surface moisture = 1%

These values are only examples and must not be used directly for production batching.

15.1 Water Contributed by Fine Aggregate

Water contributed by fine aggregate:

= 661 × 0.03

= 19.83 litres

15.2 Water Contributed by Coarse Aggregate

Water contributed by coarse aggregate:

= 1240 × 0.01

= 12.40 litres

15.3 Total Water Contributed by Aggregates

Total water:

= 19.83 + 12.40

= 32.23 litres

15.4 Plant Water to Be Added

Plant water to be added:

= External design water − Water contributed by aggregates

= 147.6 − 32.23

= 115.37 litres/m³

Therefore:

Plant water to be added ≈ 115 litres/m³

This value is valid only for the assumed free-moisture conditions and the external-water basis used in this example.

15.5 Wet Fine Aggregate Quantity

Wet fine aggregate:

= 661 × 1.03

= 680.83 kg

Therefore:

Wet fine aggregate ≈ 681 kg

15.6 Wet Coarse Aggregate Quantity

Wet coarse aggregate:

= 1240 × 1.01

= 1252.40 kg

Therefore:

Wet coarse aggregate ≈ 1252 kg

If the aggregate is below saturated surface-dry condition, additional water may be absorbed by the aggregate.

The actual absorption correction must be calculated using laboratory test results.

Free surface moisture and absorption are not the same value.

16. Trial-Mix and Quality-Control Requirements

M45 concrete requires strict control of materials, batching and testing.

Before approving the mix for production, laboratory and site trials must be conducted using the actual materials.

Check the following:

  1. Slump immediately after mixing
  2. Slump retention where delivery time is significant
  3. Concrete temperature
  4. Bleeding and segregation
  5. Fresh concrete density and yield
  6. Admixture compatibility
  7. Setting time
  8. Aggregate moisture correction
  9. Workability and finishability
  10. Cube compressive strength at specified ages
  11. Durability requirements
  12. Batch-to-batch consistency
  13. Concrete appearance and cohesiveness
  14. Final approval by the responsible engineer

Do not add unmeasured water at the site to correct slump.

Any workability adjustment must follow the approved admixture procedure and documented trial results.

Suggested Trial-Mix Record

TrialCementWaterAdmixture dosageSlumpDensity7-day strength28-day strengthRemarks
Trial 1RecordRecordRecordRecordRecordRecordRecordRecord
Trial 2RecordRecordRecordRecordRecordRecordRecordRecord
Trial 3RecordRecordRecordRecordRecordRecordRecordRecord

The final mix should be selected only after confirming the required strength, workability, durability and production consistency.

17. Common Errors to Avoid

  • Treating M45 as a nominal mix
  • Using a fixed 1:2:4 ratio for M45 concrete
  • Producing M45 by simply increasing cement in an M30 mix
  • Treating 410 kg/m³ as the cement content for every M45 mix
  • Using the same mix for different exposure conditions
  • Treating 25% water reduction as a fixed code value
  • Ignoring the water contained in liquid admixture
  • Using saturated surface-dry quantities without moisture correction
  • Adding uncontrolled water at the construction site
  • Using the 60:40 coarse-aggregate split without grading verification
  • Using assumed specific gravities for final production
  • Using the same mix for pumped concrete without a pumpability trial
  • Changing M-sand to river sand without redesigning the mix
  • Approving the mix without cube-strength verification
  • Ignoring bleeding, segregation or slump retention
  • Publishing an initial trial mix as a universal construction recipe

18. Frequently Asked Questions

Is this the final M45 concrete mix?

No. It is an illustrative initial trial mix based on stated assumptions. The final production mix requires laboratory and site verification using actual materials.

Why is 410 kg/m³ cement adopted?

For the selected very-severe-exposure RCC condition, the durability minimum is 340 kg/m³. However, the selected strength-oriented trial basis uses 147.6 litres of design water and a 0.36 water–cement ratio:

147.6 ÷ 0.36 = 410 kg/m³

Therefore, 410 kg/m³ is adopted for this initial example.

Is 410 kg/m³ cement required for every M45 mix?

No. The cement quantity depends on the target strength, water–cement ratio, exposure condition, workability, materials, admixture and trial results.

Why is the water–cement ratio 0.36?

The ratio is calculated as:

147.6 ÷ 410 = 0.36

The value is below the maximum durability limit of 0.45 for the selected exposure condition.

Can this mix be used for extreme exposure?

Not directly. Extreme exposure has more stringent durability requirements. The applicable maximum water–cement ratio, minimum cement content, grade and project specifications must be checked separately.

Is the ratio 1:1.61:3.02 a nominal mix ratio?

No. It is an approximate calculated mass-based trial proportion obtained from the absolute-volume calculation. It is not a nominal volumetric ratio.

Why is approximately 148 litres of water used?

The reference water content is adjusted for the 100 mm target slump and an illustrative superplasticizer water reduction. The design-basis value is then fixed at 147.6 litres/m³ to maintain a 0.36 ratio with 410 kg/m³ cement.

Is the 25% water reduction guaranteed?

No. It is only an illustrative assumption. Actual water reduction depends on cement chemistry, aggregate grading, admixture type, dosage, temperature, mixing conditions and required slump retention.

Can the cement quantity be reduced below 410 kg/m³?

It should not be reduced without checking the target strength, durability requirements, applicable project specifications and trial-mix results.

Can this mix be used without superplasticizer?

Not automatically. Removing the admixture may increase the water requirement and change the water–cement ratio, cement quantity, workability and strength. The mix must be redesigned and tested.

Can this mix be used for pumped concrete?

Not automatically. Pumped concrete requires separate checks for aggregate grading, paste volume, pumpability, slump retention, blockage risk and segregation resistance.

Can river sand replace M-sand directly?

No direct substitution should be made. A change in fine aggregate requires new checks for grading, moisture, absorption, workability, water demand and strength.

Is the 50-litre quantity suitable for production?

No. It is intended only for a controlled laboratory or trial batch. Production quantities require approved mix design, calibrated equipment and moisture correction.

19. Related Resources

Technical Basis and Applicable Standards

This educational example is based on the general principles of:

  • IS 10262:2019 — Concrete Mix Proportioning: Guidelines
  • IS 456:2000 — Plain and Reinforced Concrete: Code of Practice, including applicable amendments
  • IS 383:2016 — Coarse and Fine Aggregate for Concrete: Specification
  • IS 9103 — Concrete Admixtures: Specification

Always verify the latest applicable editions, amendments, project specifications and laboratory requirements before using the information for engineering work.

Conclusion

For the stated assumptions, the preliminary M45 concrete trial mix per cubic metre is:

  • OPC 53 cement: 410 kg
  • Fine aggregate: approximately 661 kg
  • Coarse aggregate: approximately 1240 kg
  • External design water: 147.6 litres
  • Practical rounded water: approximately 148 litres
  • Superplasticizer: 4.10 kg
  • Calculation-basis water–cement ratio: 0.36
  • Target slump: 100 mm
  • Approximate mass-based trial proportion: 1:1.61:3.02

These quantities are valid only for the stated materials, exposure condition, aggregate grading, specific gravities, moisture condition, admixture dosage and design assumptions.

Final approval requires trial-mix testing, cube-strength verification, durability checks and confirmation by the responsible project engineer.

About T Square Civil Engineering

T Square Civil Engineering provides practical civil-engineering explanations, concrete technology guidance, construction calculations and site-oriented learning resources.

The content connects engineering theory with construction practice, testing, quality control and field application—from Theory to Construction Practice.

Disclaimer

The information on this website is provided for educational purposes only.

It does not replace project-specific engineering design, professional advice, approved drawings or construction specifications. Examples, calculations and suggested procedures should not be adopted directly for construction without appropriate verification. Always check the latest applicable standards and amendments, local requirements, project specifications, material-test results and site conditions.

Final design, testing, acceptance and construction decisions should be made by qualified professionals and the responsible project authorities.

T Square Civil Engineering is an independent educational platform and is not affiliated with the Bureau of Indian Standards, any government authority, cement manufacturer or admixture manufacturer mentioned on this page.